Galvanic corrosion in solar mounting systems: facts, myths and the right choice of materials
When selecting materials for a mounting system, the risk of galvanic corrosion is often overlooked. When different metals are combined incorrectly, this can cause corrosion and shorten the service life of the mounting system.
Fortunately, galvanic corrosion can be avoided with the right choice of materials. Under the right conditions, aluminium and stainless steel can be used together safely.
In this article, we explain how galvanic corrosion occurs, which material combinations require attention, and what installers should look out for to safeguard the service life of their mounting system.
What is galvanic corrosion?
Galvanic corrosion occurs when two dissimilar metals are in electrical contact and a conductive liquid, such as rainwater or condensation, is present. The difference in electrode potential between the two metals triggers an electrochemical reaction.
The less noble metal acts as the anode and slowly loses material, while the more noble metal acts as the cathode and remains largely unaffected. In other words, one metal sacrifices itself for the benefit of the other.
Because solar installations are exposed to moisture for decades, it is fair for installers to ask whether this poses a risk to their mounting system.
Not every metal combination is a problem
The idea that aluminium and stainless steel should never be combined is a persistent misconception. These materials have been used together in the solar industry for many years.
What matters is choosing the right combination and the right proportions between the two materials.
ProMount deliberately combines aluminium rails and clamps with high-grade stainless steel fasteners, such as A2 (AISI 304). This combination is based on years of field experience and is designed to perform reliably throughout the entire lifetime of the installation.
The anode-to-cathode area ratio determines the risk
An aspect that is often overlooked is the surface area ratio between the two metals.
When a large aluminium surface is fixed with a small stainless steel screw or bolt, the effect of galvanic corrosion remains negligible. The small stainless steel surface barely affects the much larger aluminium component.
The reverse is less favourable. When a small aluminium component is combined with a large stainless steel surface, corrosion can progress considerably faster, especially in aggressive environments such as coastal or industrial areas.
That is why material selection in a professional mounting system is never left to chance. Dimensions, material grades and the proportions between them are carefully matched.
Why does ProMount use both aluminium and stainless steel?
A PV mounting system has to combine several properties.
Aluminium offers an excellent strength-to-weight ratio. It is lightweight, easy to process and naturally corrosion-resistant thanks to the protective oxide layer that forms on its surface.
Stainless steel is used for components that have to carry high mechanical loads, such as bolts, screws and roof hooks. Thanks to its high tensile strength and excellent corrosion resistance, stainless steel stays reliable for years, even in harsh weather conditions.
By combining both materials deliberately, you benefit from the strengths of each without amplifying their weaknesses.
Which material combinations are suitable?
Not every metal combination is equally suited to outdoor applications.
The table below shows some common metal combinations and the expected effect of galvanic corrosion in those situations.
| Profiles / roof hooks & clamps | Fastener material (bolts / nuts / screws / rivets etc.) | |||
|---|---|---|---|---|
| Galvanised steel | Aluminium | Stainless steel A2 (304) | Stainless steel A4 (316) | |
| Galvanised steel | A | C | D | D |
| Steel | B | A | C | D |
| Aluminium and aluminium alloys | C | A | C | F |
| Stainless steel 304 | B | E | A | A |
| Stainless steel 410 | B | E | A | A |
| A | The corrosion of the materials being fixed is not affected by the fastener material used. |
| B | The corrosion of the materials being fixed remains unchanged, but the surface treatment of the fastener may be damaged, exposing unprotected metal. |
| C | The corrosion of the materials being fixed increases only slightly due to the fastener material. |
| D | The corrosion of the materials being fixed may increase significantly due to the fastener material used. |
| E | The corrosion of the materials being fixed remains unchanged, while the corrosion of the fastener material increases through interaction with the materials being fixed. |
| F | Not recommended. |
Why original components matter
At first glance, a bolt is just a bolt. Yet a small change in material or alloy can have a major impact on the service life of an installation.
Original components are developed and tested as one complete system. This takes into account not only mechanical strength but also material compatibility, corrosion resistance and long-term performance.
Mixing parts from different systems, or using components of unknown material, removes that certainty. The risk of unwanted corrosion or premature wear increases as a result.
For professional installers, it is therefore advisable to always use fasteners developed specifically for the mounting system in question.
Field experience supports reliability
Although galvanic corrosion is often raised as a point of attention, years of field experience show that correctly designed mounting systems are barely affected by it.
At ProMount, we do not leave material selection to chance. We carefully match all materials and components within our mounting systems, taking into account material compatibility, corrosion resistance, mechanical strength and long-term performance. This limits the risk of galvanic corrosion and helps preserve the strength and functionality of the mounting system throughout the lifetime of the PV installation.
Conclusion
Galvanic corrosion is a technical phenomenon that every installer should take into account, but it is no reason for concern. When the right materials are combined in the right way, its impact remains minimal.
That is why we develop and test our components as one complete system. By carefully matching materials and fasteners, we take the guesswork out of material selection for installers. This gives them a strong, durable and corrosion-resistant mounting system that withstands a wide range of weather conditions for years to come.
For installers, that means one important assurance: a reliable installation that keeps performing, today and in the decades ahead.